Natnicha Pariyatdulapak, Pornkiat Churnjitapirom, T. Srikhirin, Nita Viwattanatipa
{"title":"透明矫正器材料上正畸按钮的结合强度","authors":"Natnicha Pariyatdulapak, Pornkiat Churnjitapirom, T. Srikhirin, Nita Viwattanatipa","doi":"10.1080/13440241.2021.1972243","DOIUrl":null,"url":null,"abstract":"ABSTRACT Purpose To evaluate the shear bond strength of orthodontic buttons bonded on various clear aligner materials using orthodontic plastic adhesive. Materials and methods Three types of thermoplastic materials: 1) Duran (Polyethylene terephthalate glycol), 2) Essix A+ (Polyethylene terephthalate glycol), and 3) Zendura (Polyurethane) were bonded with either metal or plastic buttons using orthodontic plastic adhesive (Bond aligner®). Six experimental groups with 15 specimens per group were prepared. Bond strength testing was done according to the Lap Shear Test Method (ASTM D3163) using the universal testing machine. Bond failure mode (modified from ASTM D5573) was examined with a stereoscope. Kruskal-Wallis and post hoc tests were used to analyse the differences in shear bond strength among the six groups. Results Mean bond strengths were as follows: 1) Duran-metal (DM) (7.04 MPa); 2) Duran-plastic (DP) (5.37 MPa); 3) Essix-metal (EM) (5.55 MPa); 4) Essix-plastic (EP) (4.62 MPa); 5) Zendura-metal (ZM) (1.17 MPa); and 6) Zendura-plastic (ZP) (1.40 MPa). Shear bond strength among the three thermoplastic materials were significantly different (p < .05). For the bond failure mode, regardless of button type, Duran and Essix A+ showed substrate failure of the thermoplastic sheet, while Zendura showed adhesive failure at the thermoplastic sheet interface. Conclusion Orthodontic buttons bonded on Duran and Essix A+ using orthodontic plastic adhesive could achieve very high bond strength that the thermoplastic sheets would tear before button detachment occurred. Buttons bonded to Zendura resulted in significantly greater bond failure rates.","PeriodicalId":43169,"journal":{"name":"Orthodontic Waves","volume":"80 1","pages":"224 - 231"},"PeriodicalIF":0.5000,"publicationDate":"2021-10-02","publicationTypes":"Journal Article","fieldsOfStudy":null,"isOpenAccess":false,"openAccessPdf":"","citationCount":"1","resultStr":"{\"title\":\"Bond strength of orthodontic buttons on clear aligner materials\",\"authors\":\"Natnicha Pariyatdulapak, Pornkiat Churnjitapirom, T. Srikhirin, Nita Viwattanatipa\",\"doi\":\"10.1080/13440241.2021.1972243\",\"DOIUrl\":null,\"url\":null,\"abstract\":\"ABSTRACT Purpose To evaluate the shear bond strength of orthodontic buttons bonded on various clear aligner materials using orthodontic plastic adhesive. Materials and methods Three types of thermoplastic materials: 1) Duran (Polyethylene terephthalate glycol), 2) Essix A+ (Polyethylene terephthalate glycol), and 3) Zendura (Polyurethane) were bonded with either metal or plastic buttons using orthodontic plastic adhesive (Bond aligner®). Six experimental groups with 15 specimens per group were prepared. Bond strength testing was done according to the Lap Shear Test Method (ASTM D3163) using the universal testing machine. Bond failure mode (modified from ASTM D5573) was examined with a stereoscope. Kruskal-Wallis and post hoc tests were used to analyse the differences in shear bond strength among the six groups. Results Mean bond strengths were as follows: 1) Duran-metal (DM) (7.04 MPa); 2) Duran-plastic (DP) (5.37 MPa); 3) Essix-metal (EM) (5.55 MPa); 4) Essix-plastic (EP) (4.62 MPa); 5) Zendura-metal (ZM) (1.17 MPa); and 6) Zendura-plastic (ZP) (1.40 MPa). Shear bond strength among the three thermoplastic materials were significantly different (p < .05). For the bond failure mode, regardless of button type, Duran and Essix A+ showed substrate failure of the thermoplastic sheet, while Zendura showed adhesive failure at the thermoplastic sheet interface. Conclusion Orthodontic buttons bonded on Duran and Essix A+ using orthodontic plastic adhesive could achieve very high bond strength that the thermoplastic sheets would tear before button detachment occurred. Buttons bonded to Zendura resulted in significantly greater bond failure rates.\",\"PeriodicalId\":43169,\"journal\":{\"name\":\"Orthodontic Waves\",\"volume\":\"80 1\",\"pages\":\"224 - 231\"},\"PeriodicalIF\":0.5000,\"publicationDate\":\"2021-10-02\",\"publicationTypes\":\"Journal Article\",\"fieldsOfStudy\":null,\"isOpenAccess\":false,\"openAccessPdf\":\"\",\"citationCount\":\"1\",\"resultStr\":null,\"platform\":\"Semanticscholar\",\"paperid\":null,\"PeriodicalName\":\"Orthodontic Waves\",\"FirstCategoryId\":\"1085\",\"ListUrlMain\":\"https://doi.org/10.1080/13440241.2021.1972243\",\"RegionNum\":0,\"RegionCategory\":null,\"ArticlePicture\":[],\"TitleCN\":null,\"AbstractTextCN\":null,\"PMCID\":null,\"EPubDate\":\"\",\"PubModel\":\"\",\"JCR\":\"Q4\",\"JCRName\":\"DENTISTRY, ORAL SURGERY & MEDICINE\",\"Score\":null,\"Total\":0}","platform":"Semanticscholar","paperid":null,"PeriodicalName":"Orthodontic Waves","FirstCategoryId":"1085","ListUrlMain":"https://doi.org/10.1080/13440241.2021.1972243","RegionNum":0,"RegionCategory":null,"ArticlePicture":[],"TitleCN":null,"AbstractTextCN":null,"PMCID":null,"EPubDate":"","PubModel":"","JCR":"Q4","JCRName":"DENTISTRY, ORAL SURGERY & MEDICINE","Score":null,"Total":0}
Bond strength of orthodontic buttons on clear aligner materials
ABSTRACT Purpose To evaluate the shear bond strength of orthodontic buttons bonded on various clear aligner materials using orthodontic plastic adhesive. Materials and methods Three types of thermoplastic materials: 1) Duran (Polyethylene terephthalate glycol), 2) Essix A+ (Polyethylene terephthalate glycol), and 3) Zendura (Polyurethane) were bonded with either metal or plastic buttons using orthodontic plastic adhesive (Bond aligner®). Six experimental groups with 15 specimens per group were prepared. Bond strength testing was done according to the Lap Shear Test Method (ASTM D3163) using the universal testing machine. Bond failure mode (modified from ASTM D5573) was examined with a stereoscope. Kruskal-Wallis and post hoc tests were used to analyse the differences in shear bond strength among the six groups. Results Mean bond strengths were as follows: 1) Duran-metal (DM) (7.04 MPa); 2) Duran-plastic (DP) (5.37 MPa); 3) Essix-metal (EM) (5.55 MPa); 4) Essix-plastic (EP) (4.62 MPa); 5) Zendura-metal (ZM) (1.17 MPa); and 6) Zendura-plastic (ZP) (1.40 MPa). Shear bond strength among the three thermoplastic materials were significantly different (p < .05). For the bond failure mode, regardless of button type, Duran and Essix A+ showed substrate failure of the thermoplastic sheet, while Zendura showed adhesive failure at the thermoplastic sheet interface. Conclusion Orthodontic buttons bonded on Duran and Essix A+ using orthodontic plastic adhesive could achieve very high bond strength that the thermoplastic sheets would tear before button detachment occurred. Buttons bonded to Zendura resulted in significantly greater bond failure rates.
期刊介绍:
Orthodontic Waves is the official publication of the Japanese Orthodontic Society. The aim of this journal is to foster the advancement of orthodontic research and practice. The journal seeks to publish original articles (i) definitive reports of wide interest to the orthodontic community, (ii) Case Reports and (iii) Short Communications. Research papers stand on the scientific basis of orthodontics. Clinical topics covered include all techniques and approaches to treatment planning. All submissions are subject to peer review.