IF 1.5 4区 医学Q3 DENTISTRY, ORAL SURGERY & MEDICINEPediatric dentistryPub Date : 2023-01-15
Julia Kai-Chin Peng, Jung-Wei Chen, Roberto Savignano, Brian Goodacre
{"title":"基于新型三维计算机断层扫描方法的预制牙冠耐磨性比较。","authors":"Julia Kai-Chin Peng, Jung-Wei Chen, Roberto Savignano, Brian Goodacre","doi":"","DOIUrl":null,"url":null,"abstract":"<p><strong>Purpose: </strong>The purpose of this study was to compare the wear resistance of stainless steel crowns, (SSCs), zirconia crowns (ZRCs), and nanohybrid crowns (NHCs) using a 3D tomography method.</p><p><strong>Methods: </strong>Prefabricated SSCs, ZRCs, and NHCs (n equals 80) were worn for 400,000 cycles, equivalent to three years of simulated clinical wear, at 50 N and 1.2 Hz using the Leinfelder-Suzuki wear tester. Wear volume, maximum wear depth, and wear surface area were computed using a 3D superimposition method and 2D imaging software. Data were statistically analyzed using one-way analysis of variance with the least significant difference post hoc test (P<0.05).</p><p><strong>Results: </strong>After a wear simulation of three years, NHCs had a 45 percent failure rate; NHCs also had the greatest wear volume loss (0.71 mm³), maximum wear depth (0.22 mm), and wear surface area (4.45 mm²). SSCs (0.23 mm³ , 0.12 mm, 2.63 mm²) and ZRCs (0.03 mm³ , 0.08 mm, 0.20 mm ²) had less wear volume, area, and depth (P<0.001). ZRCs were the most abrasive to their antagonists (P<0.001). The NHC (against SSC wearing group) had the greatest total wear facet surface area (4.43 mm²).</p><p><strong>Conclusions: </strong>Stainless steel crowns and zirconia crowns were the most wear-resistant materials. Based on these laboratory findings, in the primary dentition, nanohybrid crowns are not recommended as long-term restorations beyond 12 months (P=0.001).</p>","PeriodicalId":19863,"journal":{"name":"Pediatric dentistry","volume":"45 1","pages":"52-59"},"PeriodicalIF":1.5000,"publicationDate":"2023-01-15","publicationTypes":"Journal Article","fieldsOfStudy":null,"isOpenAccess":false,"openAccessPdf":"","citationCount":"0","resultStr":"{\"title\":\"Wear Resistance Comparison of Prefabricated Primary Crowns Using a Novel 3D Computed Tomography Method.\",\"authors\":\"Julia Kai-Chin Peng, Jung-Wei Chen, Roberto Savignano, Brian Goodacre\",\"doi\":\"\",\"DOIUrl\":null,\"url\":null,\"abstract\":\"<p><strong>Purpose: </strong>The purpose of this study was to compare the wear resistance of stainless steel crowns, (SSCs), zirconia crowns (ZRCs), and nanohybrid crowns (NHCs) using a 3D tomography method.</p><p><strong>Methods: </strong>Prefabricated SSCs, ZRCs, and NHCs (n equals 80) were worn for 400,000 cycles, equivalent to three years of simulated clinical wear, at 50 N and 1.2 Hz using the Leinfelder-Suzuki wear tester. Wear volume, maximum wear depth, and wear surface area were computed using a 3D superimposition method and 2D imaging software. Data were statistically analyzed using one-way analysis of variance with the least significant difference post hoc test (P<0.05).</p><p><strong>Results: </strong>After a wear simulation of three years, NHCs had a 45 percent failure rate; NHCs also had the greatest wear volume loss (0.71 mm³), maximum wear depth (0.22 mm), and wear surface area (4.45 mm²). SSCs (0.23 mm³ , 0.12 mm, 2.63 mm²) and ZRCs (0.03 mm³ , 0.08 mm, 0.20 mm ²) had less wear volume, area, and depth (P<0.001). ZRCs were the most abrasive to their antagonists (P<0.001). The NHC (against SSC wearing group) had the greatest total wear facet surface area (4.43 mm²).</p><p><strong>Conclusions: </strong>Stainless steel crowns and zirconia crowns were the most wear-resistant materials. Based on these laboratory findings, in the primary dentition, nanohybrid crowns are not recommended as long-term restorations beyond 12 months (P=0.001).</p>\",\"PeriodicalId\":19863,\"journal\":{\"name\":\"Pediatric dentistry\",\"volume\":\"45 1\",\"pages\":\"52-59\"},\"PeriodicalIF\":1.5000,\"publicationDate\":\"2023-01-15\",\"publicationTypes\":\"Journal Article\",\"fieldsOfStudy\":null,\"isOpenAccess\":false,\"openAccessPdf\":\"\",\"citationCount\":\"0\",\"resultStr\":null,\"platform\":\"Semanticscholar\",\"paperid\":null,\"PeriodicalName\":\"Pediatric dentistry\",\"FirstCategoryId\":\"3\",\"ListUrlMain\":\"\",\"RegionNum\":4,\"RegionCategory\":\"医学\",\"ArticlePicture\":[],\"TitleCN\":null,\"AbstractTextCN\":null,\"PMCID\":null,\"EPubDate\":\"\",\"PubModel\":\"\",\"JCR\":\"Q3\",\"JCRName\":\"DENTISTRY, ORAL SURGERY & MEDICINE\",\"Score\":null,\"Total\":0}","platform":"Semanticscholar","paperid":null,"PeriodicalName":"Pediatric dentistry","FirstCategoryId":"3","ListUrlMain":"","RegionNum":4,"RegionCategory":"医学","ArticlePicture":[],"TitleCN":null,"AbstractTextCN":null,"PMCID":null,"EPubDate":"","PubModel":"","JCR":"Q3","JCRName":"DENTISTRY, ORAL SURGERY & MEDICINE","Score":null,"Total":0}
Wear Resistance Comparison of Prefabricated Primary Crowns Using a Novel 3D Computed Tomography Method.
Purpose: The purpose of this study was to compare the wear resistance of stainless steel crowns, (SSCs), zirconia crowns (ZRCs), and nanohybrid crowns (NHCs) using a 3D tomography method.
Methods: Prefabricated SSCs, ZRCs, and NHCs (n equals 80) were worn for 400,000 cycles, equivalent to three years of simulated clinical wear, at 50 N and 1.2 Hz using the Leinfelder-Suzuki wear tester. Wear volume, maximum wear depth, and wear surface area were computed using a 3D superimposition method and 2D imaging software. Data were statistically analyzed using one-way analysis of variance with the least significant difference post hoc test (P<0.05).
Results: After a wear simulation of three years, NHCs had a 45 percent failure rate; NHCs also had the greatest wear volume loss (0.71 mm³), maximum wear depth (0.22 mm), and wear surface area (4.45 mm²). SSCs (0.23 mm³ , 0.12 mm, 2.63 mm²) and ZRCs (0.03 mm³ , 0.08 mm, 0.20 mm ²) had less wear volume, area, and depth (P<0.001). ZRCs were the most abrasive to their antagonists (P<0.001). The NHC (against SSC wearing group) had the greatest total wear facet surface area (4.43 mm²).
Conclusions: Stainless steel crowns and zirconia crowns were the most wear-resistant materials. Based on these laboratory findings, in the primary dentition, nanohybrid crowns are not recommended as long-term restorations beyond 12 months (P=0.001).
期刊介绍:
Pediatric Dentistry is the official publication of the American Academy of Pediatric Dentistry, the American Board of Pediatric Dentistry and the College of Diplomates of the American Board of Pediatric Dentistry. It is published bi-monthly and is internationally recognized as the leading journal in the area of pediatric dentistry. The journal promotes the practice, education and research specifically related to the specialty of pediatric dentistry. This peer-reviewed journal features scientific articles, case reports and abstracts of current pediatric dental research.