Corrosion studies on XD3 reinforced concrete samples prepared by using calcium nitrate as inorganic corrosion inhibitor with different superplasticizers
{"title":"Corrosion studies on XD3 reinforced concrete samples prepared by using calcium nitrate as inorganic corrosion inhibitor with different superplasticizers","authors":"S. A. Abdulsada, R. Bak, A. Heczel, T. Török","doi":"10.2478/kom-2020-0002","DOIUrl":null,"url":null,"abstract":"Abstract This research paper presents an analysis of the corrosion properties of steel-reinforced concrete samples during immersion in 3.5 wt. % NaCl aqueous solution by measuring their response both cathodic and anodic polarization in order to determine the corrosion rates in the function of their calcium nitrate inhibitor content. This cheap inorganic inhibitor was added to the concrete mix in concentrations of 1% and 3% by weight of cement in addition to two different superplasticizers (MapeiDynamon SR 31 and Oxydtron). The compressive strengths of the so prepared samples were also checked according to the relevant European standard and were within the acceptable limits, so this inhibitor does not weaken this important property of the concrete samples. The test results on steel reinforced samples immersed in 3.5 wt. % NaCl aqueous solutions at room temperature showed promising corrosion mitigating effects just after 6 months testing period. After 6 months the lower corrosion currents (i.e. better corrosion resistance) for both types of superplasticizers were observed with those samples which contained 3% calcium nitrate inhibitor. The best result was observed with sample C4 (in this case 3% calcium nitrate was added to the mixture of cement+Oxydtron superplasticizer). The advantageous inhibition mechanism of nitrate anions is also discussed and interpreted.","PeriodicalId":17911,"journal":{"name":"Koroze a ochrana materialu","volume":"64 1","pages":"11 - 18"},"PeriodicalIF":0.0000,"publicationDate":"2020-03-01","publicationTypes":"Journal Article","fieldsOfStudy":null,"isOpenAccess":false,"openAccessPdf":"","citationCount":"1","resultStr":null,"platform":"Semanticscholar","paperid":null,"PeriodicalName":"Koroze a ochrana materialu","FirstCategoryId":"1085","ListUrlMain":"https://doi.org/10.2478/kom-2020-0002","RegionNum":0,"RegionCategory":null,"ArticlePicture":[],"TitleCN":null,"AbstractTextCN":null,"PMCID":null,"EPubDate":"","PubModel":"","JCR":"Q3","JCRName":"Materials Science","Score":null,"Total":0}
引用次数: 1
Abstract
Abstract This research paper presents an analysis of the corrosion properties of steel-reinforced concrete samples during immersion in 3.5 wt. % NaCl aqueous solution by measuring their response both cathodic and anodic polarization in order to determine the corrosion rates in the function of their calcium nitrate inhibitor content. This cheap inorganic inhibitor was added to the concrete mix in concentrations of 1% and 3% by weight of cement in addition to two different superplasticizers (MapeiDynamon SR 31 and Oxydtron). The compressive strengths of the so prepared samples were also checked according to the relevant European standard and were within the acceptable limits, so this inhibitor does not weaken this important property of the concrete samples. The test results on steel reinforced samples immersed in 3.5 wt. % NaCl aqueous solutions at room temperature showed promising corrosion mitigating effects just after 6 months testing period. After 6 months the lower corrosion currents (i.e. better corrosion resistance) for both types of superplasticizers were observed with those samples which contained 3% calcium nitrate inhibitor. The best result was observed with sample C4 (in this case 3% calcium nitrate was added to the mixture of cement+Oxydtron superplasticizer). The advantageous inhibition mechanism of nitrate anions is also discussed and interpreted.
摘要本文通过测量钢筋混凝土样品的阴极和阳极极化响应,分析了钢筋混凝土样品在3.5wt.%NaCl水溶液中浸泡期间的腐蚀性能,以确定腐蚀速率与其硝酸钙缓蚀剂含量的函数关系。除了两种不同的超塑化剂(MapeiDynamon SR 31和Oxydtron)之外,还将这种廉价的无机抑制剂以水泥重量的1%和3%的浓度添加到混凝土混合物中。还根据相关欧洲标准检查了如此制备的样品的抗压强度,并且抗压强度在可接受的范围内,因此该抑制剂不会削弱混凝土样品的这一重要性能。在室温下浸泡在3.5wt.%NaCl水溶液中的钢筋样品的测试结果表明,在6个月的测试期后,具有良好的缓蚀效果。6个月后,在含有3%硝酸钙抑制剂的样品中观察到两种类型的超塑化剂的腐蚀电流较低(即耐腐蚀性较好)。用样品C4观察到最佳结果(在这种情况下,将3%的硝酸钙添加到水泥+Oxydtron高效减水剂的混合物中)。并对硝酸根阴离子的有利抑制机理进行了讨论和解释。