B. T. Ratov, V. A. Mechnik, N. A. Bondarenko, V. M. Kolodnitskyi, E. S. Gevorkyan, V. P. Nerubaskyi, A. G. Gusmanova, B. V. Fedorov, N. A. Kaldibaev, M. T. Arshidinova, V. G. Kulych
{"title":"冲击载荷作用下Сdiamond - (WC-Co) - zro2复合材料断口结构","authors":"B. T. Ratov, V. A. Mechnik, N. A. Bondarenko, V. M. Kolodnitskyi, E. S. Gevorkyan, V. P. Nerubaskyi, A. G. Gusmanova, B. V. Fedorov, N. A. Kaldibaev, M. T. Arshidinova, V. G. Kulych","doi":"10.3103/S1063457623050088","DOIUrl":null,"url":null,"abstract":"<div><div><h3>\n <b>Abstract</b>—</h3><p>The effect of the addition of ZrO<sub>2</sub> micropowder (in the range from 0 to 10%) on the structural changes of the hard alloy matrix in the area of fracture as a result of impact loading of a sample of composite diamond-containing material (DCM) 25С<sub>diamond</sub>–70.5WC‒4.5Co wt % was studied, formed by the method of spark plasma sintering in the temperature range from 20 to 1350°С at a pressure of 30 MPa for 3 min. It was found that in the DCM sample without ZrO<sub>2</sub> additive, the structure of the hard alloy matrix has the appearance characteristic of brittle fracture, which is evidenced by the smooth relief of the fracture surface. In this case, the destruction of the DCM sample occurs by chipping of the components of the hard alloy matrix, which leads to a decrease in its wear resistance. The introduction of the ZrO<sub>2</sub> additive in the amount of 4% into the composition of DCM causes a change in the structure of the fracture surface. On the fracture surface of the carbide matrix of the DCM sample, nanopores with a structural size of ~100–500 nm are formed as a result of viscous (pitting) fracture. At the same time, in addition to the formation of dimples on the fracture surface of the hard alloy matrix, a highly developed relief is simultaneously formed on the surface of the diamond grain, which is evidence of improved diamond retention and increased wear resistance of the composite. With a further increase to 10% of the ZrO<sub>2</sub> additive in the DCM composition, a more pronounced microrelief with the presence of deep dimples and microcracks is formed on the fracture surfaces of the hard alloy matrix and diamond grain. It is proposed to use the type of relief of the fracture surface of sintered DCM samples during impact fracture at room temperature as an assessment of the characteristics of the strength of diamond retention.</p></div></div>","PeriodicalId":670,"journal":{"name":"Journal of Superhard Materials","volume":"45 5","pages":"348 - 359"},"PeriodicalIF":1.2000,"publicationDate":"2023-11-13","publicationTypes":"Journal Article","fieldsOfStudy":null,"isOpenAccess":false,"openAccessPdf":"","citationCount":"0","resultStr":"{\"title\":\"Features Structure of the Сdiamond‒(WC‒Co)‒ZrO2 Composite Fracture Surface as a Result of Impact Loading\",\"authors\":\"B. T. Ratov, V. A. Mechnik, N. A. Bondarenko, V. M. Kolodnitskyi, E. S. Gevorkyan, V. P. Nerubaskyi, A. G. Gusmanova, B. V. Fedorov, N. A. Kaldibaev, M. T. Arshidinova, V. G. Kulych\",\"doi\":\"10.3103/S1063457623050088\",\"DOIUrl\":null,\"url\":null,\"abstract\":\"<div><div><h3>\\n <b>Abstract</b>—</h3><p>The effect of the addition of ZrO<sub>2</sub> micropowder (in the range from 0 to 10%) on the structural changes of the hard alloy matrix in the area of fracture as a result of impact loading of a sample of composite diamond-containing material (DCM) 25С<sub>diamond</sub>–70.5WC‒4.5Co wt % was studied, formed by the method of spark plasma sintering in the temperature range from 20 to 1350°С at a pressure of 30 MPa for 3 min. It was found that in the DCM sample without ZrO<sub>2</sub> additive, the structure of the hard alloy matrix has the appearance characteristic of brittle fracture, which is evidenced by the smooth relief of the fracture surface. In this case, the destruction of the DCM sample occurs by chipping of the components of the hard alloy matrix, which leads to a decrease in its wear resistance. The introduction of the ZrO<sub>2</sub> additive in the amount of 4% into the composition of DCM causes a change in the structure of the fracture surface. On the fracture surface of the carbide matrix of the DCM sample, nanopores with a structural size of ~100–500 nm are formed as a result of viscous (pitting) fracture. At the same time, in addition to the formation of dimples on the fracture surface of the hard alloy matrix, a highly developed relief is simultaneously formed on the surface of the diamond grain, which is evidence of improved diamond retention and increased wear resistance of the composite. With a further increase to 10% of the ZrO<sub>2</sub> additive in the DCM composition, a more pronounced microrelief with the presence of deep dimples and microcracks is formed on the fracture surfaces of the hard alloy matrix and diamond grain. It is proposed to use the type of relief of the fracture surface of sintered DCM samples during impact fracture at room temperature as an assessment of the characteristics of the strength of diamond retention.</p></div></div>\",\"PeriodicalId\":670,\"journal\":{\"name\":\"Journal of Superhard Materials\",\"volume\":\"45 5\",\"pages\":\"348 - 359\"},\"PeriodicalIF\":1.2000,\"publicationDate\":\"2023-11-13\",\"publicationTypes\":\"Journal Article\",\"fieldsOfStudy\":null,\"isOpenAccess\":false,\"openAccessPdf\":\"\",\"citationCount\":\"0\",\"resultStr\":null,\"platform\":\"Semanticscholar\",\"paperid\":null,\"PeriodicalName\":\"Journal of Superhard Materials\",\"FirstCategoryId\":\"88\",\"ListUrlMain\":\"https://link.springer.com/article/10.3103/S1063457623050088\",\"RegionNum\":4,\"RegionCategory\":\"材料科学\",\"ArticlePicture\":[],\"TitleCN\":null,\"AbstractTextCN\":null,\"PMCID\":null,\"EPubDate\":\"\",\"PubModel\":\"\",\"JCR\":\"Q4\",\"JCRName\":\"MATERIALS SCIENCE, MULTIDISCIPLINARY\",\"Score\":null,\"Total\":0}","platform":"Semanticscholar","paperid":null,"PeriodicalName":"Journal of Superhard Materials","FirstCategoryId":"88","ListUrlMain":"https://link.springer.com/article/10.3103/S1063457623050088","RegionNum":4,"RegionCategory":"材料科学","ArticlePicture":[],"TitleCN":null,"AbstractTextCN":null,"PMCID":null,"EPubDate":"","PubModel":"","JCR":"Q4","JCRName":"MATERIALS SCIENCE, MULTIDISCIPLINARY","Score":null,"Total":0}
Features Structure of the Сdiamond‒(WC‒Co)‒ZrO2 Composite Fracture Surface as a Result of Impact Loading
Abstract—
The effect of the addition of ZrO2 micropowder (in the range from 0 to 10%) on the structural changes of the hard alloy matrix in the area of fracture as a result of impact loading of a sample of composite diamond-containing material (DCM) 25Сdiamond–70.5WC‒4.5Co wt % was studied, formed by the method of spark plasma sintering in the temperature range from 20 to 1350°С at a pressure of 30 MPa for 3 min. It was found that in the DCM sample without ZrO2 additive, the structure of the hard alloy matrix has the appearance characteristic of brittle fracture, which is evidenced by the smooth relief of the fracture surface. In this case, the destruction of the DCM sample occurs by chipping of the components of the hard alloy matrix, which leads to a decrease in its wear resistance. The introduction of the ZrO2 additive in the amount of 4% into the composition of DCM causes a change in the structure of the fracture surface. On the fracture surface of the carbide matrix of the DCM sample, nanopores with a structural size of ~100–500 nm are formed as a result of viscous (pitting) fracture. At the same time, in addition to the formation of dimples on the fracture surface of the hard alloy matrix, a highly developed relief is simultaneously formed on the surface of the diamond grain, which is evidence of improved diamond retention and increased wear resistance of the composite. With a further increase to 10% of the ZrO2 additive in the DCM composition, a more pronounced microrelief with the presence of deep dimples and microcracks is formed on the fracture surfaces of the hard alloy matrix and diamond grain. It is proposed to use the type of relief of the fracture surface of sintered DCM samples during impact fracture at room temperature as an assessment of the characteristics of the strength of diamond retention.
期刊介绍:
Journal of Superhard Materials presents up-to-date results of basic and applied research on production, properties, and applications of superhard materials and related tools. It publishes the results of fundamental research on physicochemical processes of forming and growth of single-crystal, polycrystalline, and dispersed materials, diamond and diamond-like films; developments of methods for spontaneous and controlled synthesis of superhard materials and methods for static, explosive and epitaxial synthesis. The focus of the journal is large single crystals of synthetic diamonds; elite grinding powders and micron powders of synthetic diamonds and cubic boron nitride; polycrystalline and composite superhard materials based on diamond and cubic boron nitride; diamond and carbide tools for highly efficient metal-working, boring, stone-working, coal mining and geological exploration; articles of ceramic; polishing pastes for high-precision optics; precision lathes for diamond turning; technologies of precise machining of metals, glass, and ceramics. The journal covers all fundamental and technological aspects of synthesis, characterization, properties, devices and applications of these materials. The journal welcomes manuscripts from all countries in the English language.