Direselgn Molla Semanie, Lei Zhang, Hanur Meku Yesuf, Biruk Fentahun Adamu, Buguang Zhou, Jiansheng Guo
{"title":"拉伸比和触发温度对水热响应形状记忆微复合丝性能的影响","authors":"Direselgn Molla Semanie, Lei Zhang, Hanur Meku Yesuf, Biruk Fentahun Adamu, Buguang Zhou, Jiansheng Guo","doi":"10.1007/s10570-024-06146-7","DOIUrl":null,"url":null,"abstract":"<div><p>This paper investigates the production of hydrothermal responsive shape memory filaments with different draw ratios (0.8, 2.0 and 3.2) using microcrystalline cellulose (MCC) as a filler and shape memory polyurethane (SMPU) as a matrix. A mechanical-thermo-aqueous programming test was conducted to study the shape-memory properties of the microcomposite filaments. The effect of draw ratio and triggering temperature on mechanical, physical, thermal, morphological, and shape memory properties was thoroughly studied. Among the microcomposite filaments, SMPU-MCC with a draw ratio of 2.0 exhibited the highest tenacity value of 0.91 cN/dtex in its original shape with an elongation of 385.2%. The differential scanning calorimetry results showed that the glass transition temperature (T<sub>g</sub>) of the filaments increased as the draw ratio increased from 0.8 to 3.2, ranging from 38.35 to 41.02 °C. The crystallinity percentages obtained for pure SMPU, SMPU-MCC-0.8, SMPU-MCC-2.0, and SMPU-MCC-3.2 were 27.10%, 30.68%, 38.72%, and 36.88%, respectively. In addition, an optimum draw ratio led to a degradation temperature rise from 372.5 to 391.3 °C which shows the thermal stability of the filaments was significantly influenced by the intermolecular bonding between MCC and SMPU, which intensified as the draw ratio increased from 0.8 to 2.0. Moreover, the filaments exhibited excellent mechanical and thermal properties in six cycles at the optimum draw ratio and triggering temperature indicating their future application for repeated use without experiencing major changes in shape memory properties.</p></div>","PeriodicalId":511,"journal":{"name":"Cellulose","volume":"31 15","pages":"9395 - 9412"},"PeriodicalIF":4.9000,"publicationDate":"2024-09-11","publicationTypes":"Journal Article","fieldsOfStudy":null,"isOpenAccess":false,"openAccessPdf":"","citationCount":"0","resultStr":"{\"title\":\"Effect of draw ratio and triggering temperature on properties of hydrothermal responsive shape memory microcomposite filaments\",\"authors\":\"Direselgn Molla Semanie, Lei Zhang, Hanur Meku Yesuf, Biruk Fentahun Adamu, Buguang Zhou, Jiansheng Guo\",\"doi\":\"10.1007/s10570-024-06146-7\",\"DOIUrl\":null,\"url\":null,\"abstract\":\"<div><p>This paper investigates the production of hydrothermal responsive shape memory filaments with different draw ratios (0.8, 2.0 and 3.2) using microcrystalline cellulose (MCC) as a filler and shape memory polyurethane (SMPU) as a matrix. A mechanical-thermo-aqueous programming test was conducted to study the shape-memory properties of the microcomposite filaments. The effect of draw ratio and triggering temperature on mechanical, physical, thermal, morphological, and shape memory properties was thoroughly studied. Among the microcomposite filaments, SMPU-MCC with a draw ratio of 2.0 exhibited the highest tenacity value of 0.91 cN/dtex in its original shape with an elongation of 385.2%. The differential scanning calorimetry results showed that the glass transition temperature (T<sub>g</sub>) of the filaments increased as the draw ratio increased from 0.8 to 3.2, ranging from 38.35 to 41.02 °C. The crystallinity percentages obtained for pure SMPU, SMPU-MCC-0.8, SMPU-MCC-2.0, and SMPU-MCC-3.2 were 27.10%, 30.68%, 38.72%, and 36.88%, respectively. In addition, an optimum draw ratio led to a degradation temperature rise from 372.5 to 391.3 °C which shows the thermal stability of the filaments was significantly influenced by the intermolecular bonding between MCC and SMPU, which intensified as the draw ratio increased from 0.8 to 2.0. Moreover, the filaments exhibited excellent mechanical and thermal properties in six cycles at the optimum draw ratio and triggering temperature indicating their future application for repeated use without experiencing major changes in shape memory properties.</p></div>\",\"PeriodicalId\":511,\"journal\":{\"name\":\"Cellulose\",\"volume\":\"31 15\",\"pages\":\"9395 - 9412\"},\"PeriodicalIF\":4.9000,\"publicationDate\":\"2024-09-11\",\"publicationTypes\":\"Journal Article\",\"fieldsOfStudy\":null,\"isOpenAccess\":false,\"openAccessPdf\":\"\",\"citationCount\":\"0\",\"resultStr\":null,\"platform\":\"Semanticscholar\",\"paperid\":null,\"PeriodicalName\":\"Cellulose\",\"FirstCategoryId\":\"88\",\"ListUrlMain\":\"https://link.springer.com/article/10.1007/s10570-024-06146-7\",\"RegionNum\":2,\"RegionCategory\":\"工程技术\",\"ArticlePicture\":[],\"TitleCN\":null,\"AbstractTextCN\":null,\"PMCID\":null,\"EPubDate\":\"\",\"PubModel\":\"\",\"JCR\":\"Q1\",\"JCRName\":\"MATERIALS SCIENCE, PAPER & WOOD\",\"Score\":null,\"Total\":0}","platform":"Semanticscholar","paperid":null,"PeriodicalName":"Cellulose","FirstCategoryId":"88","ListUrlMain":"https://link.springer.com/article/10.1007/s10570-024-06146-7","RegionNum":2,"RegionCategory":"工程技术","ArticlePicture":[],"TitleCN":null,"AbstractTextCN":null,"PMCID":null,"EPubDate":"","PubModel":"","JCR":"Q1","JCRName":"MATERIALS SCIENCE, PAPER & WOOD","Score":null,"Total":0}
Effect of draw ratio and triggering temperature on properties of hydrothermal responsive shape memory microcomposite filaments
This paper investigates the production of hydrothermal responsive shape memory filaments with different draw ratios (0.8, 2.0 and 3.2) using microcrystalline cellulose (MCC) as a filler and shape memory polyurethane (SMPU) as a matrix. A mechanical-thermo-aqueous programming test was conducted to study the shape-memory properties of the microcomposite filaments. The effect of draw ratio and triggering temperature on mechanical, physical, thermal, morphological, and shape memory properties was thoroughly studied. Among the microcomposite filaments, SMPU-MCC with a draw ratio of 2.0 exhibited the highest tenacity value of 0.91 cN/dtex in its original shape with an elongation of 385.2%. The differential scanning calorimetry results showed that the glass transition temperature (Tg) of the filaments increased as the draw ratio increased from 0.8 to 3.2, ranging from 38.35 to 41.02 °C. The crystallinity percentages obtained for pure SMPU, SMPU-MCC-0.8, SMPU-MCC-2.0, and SMPU-MCC-3.2 were 27.10%, 30.68%, 38.72%, and 36.88%, respectively. In addition, an optimum draw ratio led to a degradation temperature rise from 372.5 to 391.3 °C which shows the thermal stability of the filaments was significantly influenced by the intermolecular bonding between MCC and SMPU, which intensified as the draw ratio increased from 0.8 to 2.0. Moreover, the filaments exhibited excellent mechanical and thermal properties in six cycles at the optimum draw ratio and triggering temperature indicating their future application for repeated use without experiencing major changes in shape memory properties.
期刊介绍:
Cellulose is an international journal devoted to the dissemination of research and scientific and technological progress in the field of cellulose and related naturally occurring polymers. The journal is concerned with the pure and applied science of cellulose and related materials, and also with the development of relevant new technologies. This includes the chemistry, biochemistry, physics and materials science of cellulose and its sources, including wood and other biomass resources, and their derivatives. Coverage extends to the conversion of these polymers and resources into manufactured goods, such as pulp, paper, textiles, and manufactured as well natural fibers, and to the chemistry of materials used in their processing. Cellulose publishes review articles, research papers, and technical notes.