Shushuai Wang, Renshu Yang, Yongliang Li, Bin Xu, Bin Lu
{"title":"风积砂胶结充填体力学和微观特性的单因素分析及相互作用项","authors":"Shushuai Wang, Renshu Yang, Yongliang Li, Bin Xu, Bin Lu","doi":"10.1007/s12613-022-2574-5","DOIUrl":null,"url":null,"abstract":"<div><p>The use of aeolian sand (AS) as an aggregate to prepare coal mine cemented filling materials can resolve the problems of gangue shortage and excessive AS deposits. Owing to the lack of research on the mechanism of cemented AS backfill (CASB), the response surface method (RSM) was adopted in this study to analyze the influence of ordinary Portland cement (PO) content (<i>x</i><sub>1</sub>), fly ash (FA)–AS (FA–AS) ratio (<i>x</i><sub>2</sub>), and concentration (<i>x</i><sub>3</sub>) on the mechanical and microscopic properties of the CASB. The hydration characteristics and internal pore structure of the backfill were assessed through thermogravimetric/derivative thermogravimetric analysis, mercury intrusion porosimetry, and scanning electron microscopy. The RSM results show that the influence of each factor and interaction term on the response values is extremely significant (except <i>x</i><sub>1</sub><i>x</i><sub>3</sub>, which had no obvious effect on the 28 d strength). The uniaxial compressive strength (UCS) increased with the PO content, FA–AS ratio, and concentration. The interaction effects of <i>x</i><sub>1</sub><i>x</i><sub>2</sub>, <i>x</i><sub>1</sub><i>x</i><sub>3</sub>, and <i>x</i><sub>2</sub><i>x</i><sub>3</sub> on the UCS at 3, 7, and 28 d were analyzed. In terms of the influence of interaction items, an improvement in one factor promoted the strengthening effect of another factor. The enhancement mechanism of the curing time, PO content, and FA–AS ratio on the backfill was reflected in the increase in hydration products and pore structure optimization. By contrast, the enhancement mechanism of the concentration was mainly the pore structure optimization. The UCS was positively correlated with weight loss and micropore content but negatively correlated with the total porosity. The <i>R</i><sup><i>2</i></sup> value of the fitting function of the strength and weight loss, micropore content, and total porosity exceeded 0.9, which improved the characterization of the enhancement mechanism of the UCS based on the thermogravimetric analysis and pore structure. This work obtained that the influence rules and mechanisms of the PO, FA–AS, concentration, and interaction terms on the mechanical properties of the CASB provided a certain theoretical and engineering guidance for CASB filling.</p></div>","PeriodicalId":14030,"journal":{"name":"International Journal of Minerals, Metallurgy, and Materials","volume":null,"pages":null},"PeriodicalIF":5.6000,"publicationDate":"2023-07-17","publicationTypes":"Journal Article","fieldsOfStudy":null,"isOpenAccess":false,"openAccessPdf":"","citationCount":"4","resultStr":"{\"title\":\"Single-factor analysis and interaction terms on the mechanical and microscopic properties of cemented aeolian sand backfill\",\"authors\":\"Shushuai Wang, Renshu Yang, Yongliang Li, Bin Xu, Bin Lu\",\"doi\":\"10.1007/s12613-022-2574-5\",\"DOIUrl\":null,\"url\":null,\"abstract\":\"<div><p>The use of aeolian sand (AS) as an aggregate to prepare coal mine cemented filling materials can resolve the problems of gangue shortage and excessive AS deposits. Owing to the lack of research on the mechanism of cemented AS backfill (CASB), the response surface method (RSM) was adopted in this study to analyze the influence of ordinary Portland cement (PO) content (<i>x</i><sub>1</sub>), fly ash (FA)–AS (FA–AS) ratio (<i>x</i><sub>2</sub>), and concentration (<i>x</i><sub>3</sub>) on the mechanical and microscopic properties of the CASB. The hydration characteristics and internal pore structure of the backfill were assessed through thermogravimetric/derivative thermogravimetric analysis, mercury intrusion porosimetry, and scanning electron microscopy. The RSM results show that the influence of each factor and interaction term on the response values is extremely significant (except <i>x</i><sub>1</sub><i>x</i><sub>3</sub>, which had no obvious effect on the 28 d strength). The uniaxial compressive strength (UCS) increased with the PO content, FA–AS ratio, and concentration. The interaction effects of <i>x</i><sub>1</sub><i>x</i><sub>2</sub>, <i>x</i><sub>1</sub><i>x</i><sub>3</sub>, and <i>x</i><sub>2</sub><i>x</i><sub>3</sub> on the UCS at 3, 7, and 28 d were analyzed. In terms of the influence of interaction items, an improvement in one factor promoted the strengthening effect of another factor. The enhancement mechanism of the curing time, PO content, and FA–AS ratio on the backfill was reflected in the increase in hydration products and pore structure optimization. By contrast, the enhancement mechanism of the concentration was mainly the pore structure optimization. The UCS was positively correlated with weight loss and micropore content but negatively correlated with the total porosity. The <i>R</i><sup><i>2</i></sup> value of the fitting function of the strength and weight loss, micropore content, and total porosity exceeded 0.9, which improved the characterization of the enhancement mechanism of the UCS based on the thermogravimetric analysis and pore structure. This work obtained that the influence rules and mechanisms of the PO, FA–AS, concentration, and interaction terms on the mechanical properties of the CASB provided a certain theoretical and engineering guidance for CASB filling.</p></div>\",\"PeriodicalId\":14030,\"journal\":{\"name\":\"International Journal of Minerals, Metallurgy, and Materials\",\"volume\":null,\"pages\":null},\"PeriodicalIF\":5.6000,\"publicationDate\":\"2023-07-17\",\"publicationTypes\":\"Journal Article\",\"fieldsOfStudy\":null,\"isOpenAccess\":false,\"openAccessPdf\":\"\",\"citationCount\":\"4\",\"resultStr\":null,\"platform\":\"Semanticscholar\",\"paperid\":null,\"PeriodicalName\":\"International Journal of Minerals, Metallurgy, and Materials\",\"FirstCategoryId\":\"5\",\"ListUrlMain\":\"https://link.springer.com/article/10.1007/s12613-022-2574-5\",\"RegionNum\":2,\"RegionCategory\":\"材料科学\",\"ArticlePicture\":[],\"TitleCN\":null,\"AbstractTextCN\":null,\"PMCID\":null,\"EPubDate\":\"\",\"PubModel\":\"\",\"JCR\":\"Q2\",\"JCRName\":\"MATERIALS SCIENCE, MULTIDISCIPLINARY\",\"Score\":null,\"Total\":0}","platform":"Semanticscholar","paperid":null,"PeriodicalName":"International Journal of Minerals, Metallurgy, and Materials","FirstCategoryId":"5","ListUrlMain":"https://link.springer.com/article/10.1007/s12613-022-2574-5","RegionNum":2,"RegionCategory":"材料科学","ArticlePicture":[],"TitleCN":null,"AbstractTextCN":null,"PMCID":null,"EPubDate":"","PubModel":"","JCR":"Q2","JCRName":"MATERIALS SCIENCE, MULTIDISCIPLINARY","Score":null,"Total":0}
Single-factor analysis and interaction terms on the mechanical and microscopic properties of cemented aeolian sand backfill
The use of aeolian sand (AS) as an aggregate to prepare coal mine cemented filling materials can resolve the problems of gangue shortage and excessive AS deposits. Owing to the lack of research on the mechanism of cemented AS backfill (CASB), the response surface method (RSM) was adopted in this study to analyze the influence of ordinary Portland cement (PO) content (x1), fly ash (FA)–AS (FA–AS) ratio (x2), and concentration (x3) on the mechanical and microscopic properties of the CASB. The hydration characteristics and internal pore structure of the backfill were assessed through thermogravimetric/derivative thermogravimetric analysis, mercury intrusion porosimetry, and scanning electron microscopy. The RSM results show that the influence of each factor and interaction term on the response values is extremely significant (except x1x3, which had no obvious effect on the 28 d strength). The uniaxial compressive strength (UCS) increased with the PO content, FA–AS ratio, and concentration. The interaction effects of x1x2, x1x3, and x2x3 on the UCS at 3, 7, and 28 d were analyzed. In terms of the influence of interaction items, an improvement in one factor promoted the strengthening effect of another factor. The enhancement mechanism of the curing time, PO content, and FA–AS ratio on the backfill was reflected in the increase in hydration products and pore structure optimization. By contrast, the enhancement mechanism of the concentration was mainly the pore structure optimization. The UCS was positively correlated with weight loss and micropore content but negatively correlated with the total porosity. The R2 value of the fitting function of the strength and weight loss, micropore content, and total porosity exceeded 0.9, which improved the characterization of the enhancement mechanism of the UCS based on the thermogravimetric analysis and pore structure. This work obtained that the influence rules and mechanisms of the PO, FA–AS, concentration, and interaction terms on the mechanical properties of the CASB provided a certain theoretical and engineering guidance for CASB filling.
期刊介绍:
International Journal of Minerals, Metallurgy and Materials (Formerly known as Journal of University of Science and Technology Beijing, Mineral, Metallurgy, Material) provides an international medium for the publication of theoretical and experimental studies related to the fields of Minerals, Metallurgy and Materials. Papers dealing with minerals processing, mining, mine safety, environmental pollution and protection of mines, process metallurgy, metallurgical physical chemistry, structure and physical properties of materials, corrosion and resistance of materials, are viewed as suitable for publication.