{"title":"浸没量热法测定碳块体的能量特性和微孔体积","authors":"J. Moreno-Piraján, L. Giraldo, D. P. Vargas","doi":"10.1155/2012/976275","DOIUrl":null,"url":null,"abstract":"Activated carbon monoliths disc and honeycomb type were prepared by chemical activation of coconut shell with zinc chloride at different concentrations, without using a binder. The structures were characterized by N2 adsorption at 77 K and immersion calorimetry into benzene. The experimental results showed that the activation with zinc chloride produces a wide microporous development, with micropore volume between 0,38 and 0,79 cm3g-1, apparent BET surface area between 725 and 1523 m2g-1 and immersion enthalpy between 73,5 and 164,2 Jg-1. We compared the experimental enthalpy with calculated enthalpy by equation Stoeckli-Kraehenbuehl finding a data dispersion from which can infer that the structures are not purely microporous; this fact is ratified with similar behavior that the evidence t the product EoWo.","PeriodicalId":11519,"journal":{"name":"E-journal of Chemistry","volume":null,"pages":null},"PeriodicalIF":0.0000,"publicationDate":"2012-01-01","publicationTypes":"Journal Article","fieldsOfStudy":null,"isOpenAccess":false,"openAccessPdf":"https://sci-hub-pdf.com/10.1155/2012/976275","citationCount":"4","resultStr":"{\"title\":\"Determination of Energy Characteristic and Microporous Volume by Immersion Calorimetry in Carbon Monoliths\",\"authors\":\"J. Moreno-Piraján, L. Giraldo, D. P. Vargas\",\"doi\":\"10.1155/2012/976275\",\"DOIUrl\":null,\"url\":null,\"abstract\":\"Activated carbon monoliths disc and honeycomb type were prepared by chemical activation of coconut shell with zinc chloride at different concentrations, without using a binder. The structures were characterized by N2 adsorption at 77 K and immersion calorimetry into benzene. The experimental results showed that the activation with zinc chloride produces a wide microporous development, with micropore volume between 0,38 and 0,79 cm3g-1, apparent BET surface area between 725 and 1523 m2g-1 and immersion enthalpy between 73,5 and 164,2 Jg-1. We compared the experimental enthalpy with calculated enthalpy by equation Stoeckli-Kraehenbuehl finding a data dispersion from which can infer that the structures are not purely microporous; this fact is ratified with similar behavior that the evidence t the product EoWo.\",\"PeriodicalId\":11519,\"journal\":{\"name\":\"E-journal of Chemistry\",\"volume\":null,\"pages\":null},\"PeriodicalIF\":0.0000,\"publicationDate\":\"2012-01-01\",\"publicationTypes\":\"Journal Article\",\"fieldsOfStudy\":null,\"isOpenAccess\":false,\"openAccessPdf\":\"https://sci-hub-pdf.com/10.1155/2012/976275\",\"citationCount\":\"4\",\"resultStr\":null,\"platform\":\"Semanticscholar\",\"paperid\":null,\"PeriodicalName\":\"E-journal of Chemistry\",\"FirstCategoryId\":\"1085\",\"ListUrlMain\":\"https://doi.org/10.1155/2012/976275\",\"RegionNum\":0,\"RegionCategory\":null,\"ArticlePicture\":[],\"TitleCN\":null,\"AbstractTextCN\":null,\"PMCID\":null,\"EPubDate\":\"\",\"PubModel\":\"\",\"JCR\":\"\",\"JCRName\":\"\",\"Score\":null,\"Total\":0}","platform":"Semanticscholar","paperid":null,"PeriodicalName":"E-journal of Chemistry","FirstCategoryId":"1085","ListUrlMain":"https://doi.org/10.1155/2012/976275","RegionNum":0,"RegionCategory":null,"ArticlePicture":[],"TitleCN":null,"AbstractTextCN":null,"PMCID":null,"EPubDate":"","PubModel":"","JCR":"","JCRName":"","Score":null,"Total":0}
Determination of Energy Characteristic and Microporous Volume by Immersion Calorimetry in Carbon Monoliths
Activated carbon monoliths disc and honeycomb type were prepared by chemical activation of coconut shell with zinc chloride at different concentrations, without using a binder. The structures were characterized by N2 adsorption at 77 K and immersion calorimetry into benzene. The experimental results showed that the activation with zinc chloride produces a wide microporous development, with micropore volume between 0,38 and 0,79 cm3g-1, apparent BET surface area between 725 and 1523 m2g-1 and immersion enthalpy between 73,5 and 164,2 Jg-1. We compared the experimental enthalpy with calculated enthalpy by equation Stoeckli-Kraehenbuehl finding a data dispersion from which can infer that the structures are not purely microporous; this fact is ratified with similar behavior that the evidence t the product EoWo.