{"title":"Depth profiles of akaganéite, goethite and maghemite on A1010, HPS and weathering steel panels after wet-dry corrosion tests","authors":"Jerzy A. Sawicki","doi":"10.1080/1478422X.2023.2247666","DOIUrl":null,"url":null,"abstract":"ABSTRACT The panels of high chromium steel (A1010), high-performance steel (HPS 70W) and weathering steel (WS) were exposed to accelerated salt-spray corrosion test for 1 week and to less aggressive test for additional 13 weeks. After the tests, the corrosion products formed were extracted layer after layer and examined as a function of their depth with Mössbauer transmission spectroscopy. In the case of A1010 steel, the amounts of goethite (α-FeOOH) and akaganéite (β-FeOOH) were almost equal along the depth of the corroded layer up to ∼20 μm. The rust layers on HPS and WS panels were much thicker, respectively up to ∼0.6 mm and ∼1 mm, poorly adherent and contained mostly akaganéite near the metal–rust interface, α-FeOOH increasingly further away, and – after long exposure – also up to 20% Fe as maghemite (γ-Fe2O3). Formation of β-FeOOH near the interface was promoted by chloride concentrated by spray-dry cycles. The microstructure and depth profiles of identified species, and especially the role of β-FeOOH, are discussed.","PeriodicalId":10711,"journal":{"name":"Corrosion Engineering, Science and Technology","volume":"58 1","pages":"687 - 695"},"PeriodicalIF":1.5000,"publicationDate":"2023-09-07","publicationTypes":"Journal Article","fieldsOfStudy":null,"isOpenAccess":false,"openAccessPdf":"","citationCount":"0","resultStr":null,"platform":"Semanticscholar","paperid":null,"PeriodicalName":"Corrosion Engineering, Science and Technology","FirstCategoryId":"88","ListUrlMain":"https://doi.org/10.1080/1478422X.2023.2247666","RegionNum":4,"RegionCategory":"材料科学","ArticlePicture":[],"TitleCN":null,"AbstractTextCN":null,"PMCID":null,"EPubDate":"","PubModel":"","JCR":"Q4","JCRName":"MATERIALS SCIENCE, MULTIDISCIPLINARY","Score":null,"Total":0}
引用次数: 0
Abstract
ABSTRACT The panels of high chromium steel (A1010), high-performance steel (HPS 70W) and weathering steel (WS) were exposed to accelerated salt-spray corrosion test for 1 week and to less aggressive test for additional 13 weeks. After the tests, the corrosion products formed were extracted layer after layer and examined as a function of their depth with Mössbauer transmission spectroscopy. In the case of A1010 steel, the amounts of goethite (α-FeOOH) and akaganéite (β-FeOOH) were almost equal along the depth of the corroded layer up to ∼20 μm. The rust layers on HPS and WS panels were much thicker, respectively up to ∼0.6 mm and ∼1 mm, poorly adherent and contained mostly akaganéite near the metal–rust interface, α-FeOOH increasingly further away, and – after long exposure – also up to 20% Fe as maghemite (γ-Fe2O3). Formation of β-FeOOH near the interface was promoted by chloride concentrated by spray-dry cycles. The microstructure and depth profiles of identified species, and especially the role of β-FeOOH, are discussed.
期刊介绍:
Corrosion Engineering, Science and Technology provides broad international coverage of research and practice in corrosion processes and corrosion control. Peer-reviewed contributions address all aspects of corrosion engineering and corrosion science; there is strong emphasis on effective design and materials selection to combat corrosion and the journal carries failure case studies to further knowledge in these areas.