Analysis of the reasons for the formation of defects in the 12-Cr18-Ni10-Ti steel billets and development of recommendations for its elimination

IF 0.4 Q4 METALLURGY & METALLURGICAL ENGINEERING Obrabotka Metallov-Metal Working and Material Science Pub Date : 2023-03-15 DOI:10.17212/1994-6309-2023-25.1-6-15
S. Ryaboshuk, P. Kovalev
{"title":"Analysis of the reasons for the formation of defects in the 12-Cr18-Ni10-Ti steel billets and development of recommendations for its elimination","authors":"S. Ryaboshuk, P. Kovalev","doi":"10.17212/1994-6309-2023-25.1-6-15","DOIUrl":null,"url":null,"abstract":"Introdution. Austenitic steel (e.g., AISI 304, AISI 321, AISI 316, AISI 403, 12-Cr18-Ni10-Ti, etc.) is widespread, which is caused by high corrosion resistance and the corresponding possibility of use in aggressive media. The following most common types of 12-Cr18-Ni10-Ti steel defects can be distinguished: integranular corrosion, martensitic orientation of the α-phase and ferrite δ-phase. The purpose of work: to analyze the defects formation reasons of the 12-Cr18-Ni10-Ti steel grade billets and to develop recommendations for their elimination. The methods of investigation. Tests of 12-Cr18-Ni10-Ti steel samples for resistance to integranular corrosion, metallographic analysis of defects were carried out in this work. Hardness measurements were carried out for various degrees of billets reduction. Thermodynamic calculations of phase equilibrium in multicomponent steel for different temperatures were performed by the Thermo-Calc software. Results and Discussion. It is determined that in order to prevent integranular corrosion, it is necessary to reduce the nitrogen and carbon content in steel at the stage of ladle refining to 0.05%, and also to ensure the concentration of titanium in steel is not less than the permissible value — 0.3%. These measures contribute to the reduction of Cr23C6 chromium carbides responsible for integranular corrosion. It is necessary to reduce the degree of compression of the billets to a level of no more than 50% to prevent the appearance of a ferromagnetic martensitic α-phase, since the formation of this defect is associated with a high degree of compression during drawing. The high-temperature phase of δ-ferrite exists in the metal structure in a wide temperature range. Reducing this range to 100 degrees or less by optimizing the composition of the carbon and chromium alloy in accordance with GOST 5632-2014 leads to a significant reduction of the amount of ferrite. However, it is not possible to completely eliminate it from the structure of steel. For all cases, it is necessary to assign austenization of billets in the temperature range of 1,050…1,100 °C.","PeriodicalId":42889,"journal":{"name":"Obrabotka Metallov-Metal Working and Material Science","volume":" ","pages":""},"PeriodicalIF":0.4000,"publicationDate":"2023-03-15","publicationTypes":"Journal Article","fieldsOfStudy":null,"isOpenAccess":false,"openAccessPdf":"","citationCount":"0","resultStr":null,"platform":"Semanticscholar","paperid":null,"PeriodicalName":"Obrabotka Metallov-Metal Working and Material Science","FirstCategoryId":"1085","ListUrlMain":"https://doi.org/10.17212/1994-6309-2023-25.1-6-15","RegionNum":0,"RegionCategory":null,"ArticlePicture":[],"TitleCN":null,"AbstractTextCN":null,"PMCID":null,"EPubDate":"","PubModel":"","JCR":"Q4","JCRName":"METALLURGY & METALLURGICAL ENGINEERING","Score":null,"Total":0}
引用次数: 0

Abstract

Introdution. Austenitic steel (e.g., AISI 304, AISI 321, AISI 316, AISI 403, 12-Cr18-Ni10-Ti, etc.) is widespread, which is caused by high corrosion resistance and the corresponding possibility of use in aggressive media. The following most common types of 12-Cr18-Ni10-Ti steel defects can be distinguished: integranular corrosion, martensitic orientation of the α-phase and ferrite δ-phase. The purpose of work: to analyze the defects formation reasons of the 12-Cr18-Ni10-Ti steel grade billets and to develop recommendations for their elimination. The methods of investigation. Tests of 12-Cr18-Ni10-Ti steel samples for resistance to integranular corrosion, metallographic analysis of defects were carried out in this work. Hardness measurements were carried out for various degrees of billets reduction. Thermodynamic calculations of phase equilibrium in multicomponent steel for different temperatures were performed by the Thermo-Calc software. Results and Discussion. It is determined that in order to prevent integranular corrosion, it is necessary to reduce the nitrogen and carbon content in steel at the stage of ladle refining to 0.05%, and also to ensure the concentration of titanium in steel is not less than the permissible value — 0.3%. These measures contribute to the reduction of Cr23C6 chromium carbides responsible for integranular corrosion. It is necessary to reduce the degree of compression of the billets to a level of no more than 50% to prevent the appearance of a ferromagnetic martensitic α-phase, since the formation of this defect is associated with a high degree of compression during drawing. The high-temperature phase of δ-ferrite exists in the metal structure in a wide temperature range. Reducing this range to 100 degrees or less by optimizing the composition of the carbon and chromium alloy in accordance with GOST 5632-2014 leads to a significant reduction of the amount of ferrite. However, it is not possible to completely eliminate it from the structure of steel. For all cases, it is necessary to assign austenization of billets in the temperature range of 1,050…1,100 °C.
查看原文
分享 分享
微信好友 朋友圈 QQ好友 复制链接
本刊更多论文
12-Cr18-Ni10-Ti钢坯缺陷形成原因分析及消除建议
简介。奥氏体钢(例如AISI 304、AISI 321、AISI 316、AISI 403、12-Cr18-Ni10-Ti等)广泛使用,这是由于高耐腐蚀性和在腐蚀性介质中使用的相应可能性造成的。12-Cr18-Ni10-Ti钢最常见的缺陷类型可分为:整体腐蚀、α相和铁素体δ相的马氏体取向。工作目的:分析12-Cr18-Ni10-Ti钢级钢坯缺陷形成的原因,并提出消除缺陷的建议。调查方法。本文对12-Cr18-Ni10-Ti钢试样进行了抗整体腐蚀试验,并对缺陷进行了金相分析。对不同程度的坯料还原度进行了硬度测量。使用Thermo-Calc软件对不同温度下多组分钢的相平衡进行了热力学计算。结果和讨论。确定为防止整体晶粒腐蚀,必须在钢包精炼阶段将钢中的氮和碳含量降低到0.05%,并确保钢中钛的浓度不低于允许值0.3%。这些措施有助于减少导致整体晶粒腐蚀的Cr23C6铬碳化物。有必要将坯料的压缩程度降低到不超过50%的水平,以防止出现铁磁马氏体α相,因为这种缺陷的形成与拉伸过程中的高度压缩有关。δ-铁氧体的高温相存在于金属结构中,温度范围很宽。根据GOST 5632-2014,通过优化碳和铬合金的成分,将该范围降低到100度或更低,可显著减少铁素体的量。然而,不可能将其从钢结构中完全消除。在所有情况下,有必要在1050…1100°C的温度范围内对钢坯进行奥氏体化。
本文章由计算机程序翻译,如有差异,请以英文原文为准。
求助全文
约1分钟内获得全文 去求助
来源期刊
Obrabotka Metallov-Metal Working and Material Science
Obrabotka Metallov-Metal Working and Material Science METALLURGY & METALLURGICAL ENGINEERING-
CiteScore
1.10
自引率
50.00%
发文量
26
期刊最新文献
Free vibration and mechanical behavior of treated woven jute polymer composite Analysis of mechanical behavior and free vibration characteristics of treated Saccharum munja fiber polymer composite Synthesis of Ti–Fe intermetallic compounds from elemental powders mixtures The concept of microsimulation of processes of joining dissimilar materials by plastic deformation Experimental studies of high-speed grinding rails modes
×
引用
GB/T 7714-2015
复制
MLA
复制
APA
复制
导出至
BibTeX EndNote RefMan NoteFirst NoteExpress
×
×
提示
您的信息不完整,为了账户安全,请先补充。
现在去补充
×
提示
您因"违规操作"
具体请查看互助需知
我知道了
×
提示
现在去查看 取消
×
提示
确定
0
微信
客服QQ
Book学术公众号 扫码关注我们
反馈
×
意见反馈
请填写您的意见或建议
请填写您的手机或邮箱
已复制链接
已复制链接
快去分享给好友吧!
我知道了
×
扫码分享
扫码分享
Book学术官方微信
Book学术文献互助
Book学术文献互助群
群 号:481959085
Book学术
文献互助 智能选刊 最新文献 互助须知 联系我们:info@booksci.cn
Book学术提供免费学术资源搜索服务,方便国内外学者检索中英文文献。致力于提供最便捷和优质的服务体验。
Copyright © 2023 Book学术 All rights reserved.
ghs 京公网安备 11010802042870号 京ICP备2023020795号-1