Corrosion by “Green Death” in Reboiler Bypass Duct Damper in Power-Generation Plant

{"title":"Corrosion by “Green Death” in Reboiler Bypass Duct Damper in Power-Generation Plant","authors":"","doi":"10.31399/asm.fach.modes.c0091330","DOIUrl":null,"url":null,"abstract":"\n At a power plant, C-276 nickel alloy welds (N10276) on a C-276 duct floor completely disappeared in less than half a year. A continuous supply of flue gas came in contact with the closed bypass duct. The unscrubbed combustion products condensed on the cold duct, then the closed damper conducted heat from the chimney and reheated the condensate. Investigation (visual inspection and welded coupon testing) supported the conclusion that the corrosion was caused by “Green Death,” a corrosive medium used to test for pitting resistance (11.9% H2SO4 + 1.3% HCl + 1% FeCl3 + 1% CuCl2) at 103 deg C (217 deg F). Such conditions exist at power plants. Recommendations included repairing the C-276 plates with a 686CPT weld alloy, and if that did not correct the situation, replacing the plates with 686 plate (N06686) welded with 686 CPT.","PeriodicalId":231268,"journal":{"name":"ASM Failure Analysis Case Histories: Failure Modes and Mechanisms","volume":"40 1","pages":"0"},"PeriodicalIF":0.0000,"publicationDate":"2019-06-01","publicationTypes":"Journal Article","fieldsOfStudy":null,"isOpenAccess":false,"openAccessPdf":"","citationCount":"0","resultStr":null,"platform":"Semanticscholar","paperid":null,"PeriodicalName":"ASM Failure Analysis Case Histories: Failure Modes and Mechanisms","FirstCategoryId":"1085","ListUrlMain":"https://doi.org/10.31399/asm.fach.modes.c0091330","RegionNum":0,"RegionCategory":null,"ArticlePicture":[],"TitleCN":null,"AbstractTextCN":null,"PMCID":null,"EPubDate":"","PubModel":"","JCR":"","JCRName":"","Score":null,"Total":0}
引用次数: 0

Abstract

At a power plant, C-276 nickel alloy welds (N10276) on a C-276 duct floor completely disappeared in less than half a year. A continuous supply of flue gas came in contact with the closed bypass duct. The unscrubbed combustion products condensed on the cold duct, then the closed damper conducted heat from the chimney and reheated the condensate. Investigation (visual inspection and welded coupon testing) supported the conclusion that the corrosion was caused by “Green Death,” a corrosive medium used to test for pitting resistance (11.9% H2SO4 + 1.3% HCl + 1% FeCl3 + 1% CuCl2) at 103 deg C (217 deg F). Such conditions exist at power plants. Recommendations included repairing the C-276 plates with a 686CPT weld alloy, and if that did not correct the situation, replacing the plates with 686 plate (N06686) welded with 686 CPT.
查看原文
分享 分享
微信好友 朋友圈 QQ好友 复制链接
本刊更多论文
电厂再沸器旁通风道阻尼器“绿死”腐蚀
在某电厂,C-276管道地板上的C-276镍合金焊缝(N10276)在不到半年的时间内完全消失。连续供应的烟气与封闭的旁路管道接触。未擦洗的燃烧产物在冷管道上凝结,然后关闭的阻尼器从烟囱传导热量并重新加热冷凝物。调查(目视检查和焊接接头测试)支持腐蚀是由“绿死”引起的结论,这是一种腐蚀性介质,用于测试103摄氏度(217华氏度)下的耐点蚀性(11.9% H2SO4 + 1.3% HCl + 1% FeCl3 + 1% CuCl2)。这种情况在发电厂存在。建议包括用686CPT焊接合金修复C-276板,如果不能纠正这种情况,用686CPT焊接的686板(N06686)代替。
本文章由计算机程序翻译,如有差异,请以英文原文为准。
求助全文
约1分钟内获得全文 去求助
来源期刊
自引率
0.00%
发文量
0
期刊最新文献
Fatigue Failures, With Special Reference to Fracture Characteristics Dezincification of a Copper Pipe Welded Joint Electron Fractography Pinpoints Cause of Fatigue Fracture Failure of a Hard-Faced Stainless Steel Pump Sleeve Because of Abrasive Wear by River-Water Silt Fatigue Fracture and Weld
×
引用
GB/T 7714-2015
复制
MLA
复制
APA
复制
导出至
BibTeX EndNote RefMan NoteFirst NoteExpress
×
×
提示
您的信息不完整,为了账户安全,请先补充。
现在去补充
×
提示
您因"违规操作"
具体请查看互助需知
我知道了
×
提示
现在去查看 取消
×
提示
确定
0
微信
客服QQ
Book学术公众号 扫码关注我们
反馈
×
意见反馈
请填写您的意见或建议
请填写您的手机或邮箱
已复制链接
已复制链接
快去分享给好友吧!
我知道了
×
扫码分享
扫码分享
Book学术官方微信
Book学术文献互助
Book学术文献互助群
群 号:481959085
Book学术
文献互助 智能选刊 最新文献 互助须知 联系我们:info@booksci.cn
Book学术提供免费学术资源搜索服务,方便国内外学者检索中英文文献。致力于提供最便捷和优质的服务体验。
Copyright © 2023 Book学术 All rights reserved.
ghs 京公网安备 11010802042870号 京ICP备2023020795号-1