Examination of surface defects induced during hot rolling of high-alloy steel bar and rod

K. Barlow, P. Lancaster, R. Maddison
{"title":"Examination of surface defects induced during hot rolling of high-alloy steel bar and rod","authors":"K. Barlow, P. Lancaster, R. Maddison","doi":"10.1179/030716984803275214","DOIUrl":null,"url":null,"abstract":"AbstractThe authors examine three problems associated with the production of high-alloy steel bar and rod by rolling in hand-operated mills. An outline is given of the mechanics of formation of surface defects and, by using a model material for hot steel (Plasticine) as well as three grades of steel, the defects were examined. Although the work was carried out using hand-operated mills, the conclusions drawn are relevant to commercial continuous mills for producing low-alloy and carbon steel rod and bar. The defects examined were cracking, split ends, and decarburization. The main conclusion is that careful selection of pass sequence, taking into account all the manufacturing and product requirements, is essential in order to control the rate of rejection of rod and bar with these defects","PeriodicalId":18409,"journal":{"name":"Metals technology","volume":"261 1","pages":"14-19"},"PeriodicalIF":0.0000,"publicationDate":"1984-01-01","publicationTypes":"Journal Article","fieldsOfStudy":null,"isOpenAccess":false,"openAccessPdf":"","citationCount":"12","resultStr":null,"platform":"Semanticscholar","paperid":null,"PeriodicalName":"Metals technology","FirstCategoryId":"1085","ListUrlMain":"https://doi.org/10.1179/030716984803275214","RegionNum":0,"RegionCategory":null,"ArticlePicture":[],"TitleCN":null,"AbstractTextCN":null,"PMCID":null,"EPubDate":"","PubModel":"","JCR":"","JCRName":"","Score":null,"Total":0}
引用次数: 12

Abstract

AbstractThe authors examine three problems associated with the production of high-alloy steel bar and rod by rolling in hand-operated mills. An outline is given of the mechanics of formation of surface defects and, by using a model material for hot steel (Plasticine) as well as three grades of steel, the defects were examined. Although the work was carried out using hand-operated mills, the conclusions drawn are relevant to commercial continuous mills for producing low-alloy and carbon steel rod and bar. The defects examined were cracking, split ends, and decarburization. The main conclusion is that careful selection of pass sequence, taking into account all the manufacturing and product requirements, is essential in order to control the rate of rejection of rod and bar with these defects
查看原文
分享 分享
微信好友 朋友圈 QQ好友 复制链接
本刊更多论文
高合金棒材和棒材热轧过程中表面缺陷的检测
摘要本文探讨了手工轧机生产高合金钢棒材和棒材时存在的三个问题。概述了表面缺陷的形成机制,并通过使用热钢模型材料(橡皮泥)和三种等级的钢,对缺陷进行了检查。虽然这项工作是在手工操作的轧机上进行的,但得出的结论与生产低合金和碳钢棒材的商业连续轧机有关。检查的缺陷是裂纹、分叉和脱碳。主要结论是,考虑到所有制造和产品要求,仔细选择合格顺序对于控制具有这些缺陷的棒材和棒材的废品率至关重要
本文章由计算机程序翻译,如有差异,请以英文原文为准。
求助全文
约1分钟内获得全文 去求助
来源期刊
自引率
0.00%
发文量
0
期刊最新文献
INVESTIGATION OF FRICTION EFFECT ON STRESS-STRAIN STATE OF METAL DURING FORGING OF RODS ON LEVER RADIAL- FORGING MACHINE ESTIMATION OF POWER PARAMETERS OF MSR TECHNOLOGY IMPLEMENTATION UNDER CONDITIONS OF CONTINUOUS CASTING SECTION MACHINE WITH ADDITIONAL SHEAR EFFECT Effects of Q&P Processing Conditions on Austenite Carbon Enrichment Studied by In Situ High-Energy X-ray Diffraction Experiments Optimization of high-temperature compression of as-cast Al–Cu eutectic alloy Examination of surface defects induced during hot rolling of high-alloy steel bar and rod
×
引用
GB/T 7714-2015
复制
MLA
复制
APA
复制
导出至
BibTeX EndNote RefMan NoteFirst NoteExpress
×
×
提示
您的信息不完整,为了账户安全,请先补充。
现在去补充
×
提示
您因"违规操作"
具体请查看互助需知
我知道了
×
提示
现在去查看 取消
×
提示
确定
0
微信
客服QQ
Book学术公众号 扫码关注我们
反馈
×
意见反馈
请填写您的意见或建议
请填写您的手机或邮箱
已复制链接
已复制链接
快去分享给好友吧!
我知道了
×
扫码分享
扫码分享
Book学术官方微信
Book学术文献互助
Book学术文献互助群
群 号:481959085
Book学术
文献互助 智能选刊 最新文献 互助须知 联系我们:info@booksci.cn
Book学术提供免费学术资源搜索服务,方便国内外学者检索中英文文献。致力于提供最便捷和优质的服务体验。
Copyright © 2023 Book学术 All rights reserved.
ghs 京公网安备 11010802042870号 京ICP备2023020795号-1