{"title":"模具复合组分对环氧封装器件中金铝键湿致降解的影响","authors":"A. Gallo","doi":"10.1109/RELPHY.1990.66095","DOIUrl":null,"url":null,"abstract":"Degradation of the intermetallic region of the gold wire-aluminium bonding pad interface of several types of IC devices in plastic packages is accelerated by moisture at relatively low temperatures (121-135 degrees C), leading to near-complete loss of strength after 300-400 h of autoclave testing. Measurement of bonding strength as a function of steam-autoclave time in a designed experiment shows that one common component of semiconductor molding compounds (Sb/sub 2/O/sub 3/) is the overriding factor in causing ball-lift. In support of this conclusion, a variety of brominated flame retardants, including those that claimed to be more stable to Br release, were tested in similar formulations and all were found to give ball-bond degradation, to about the same degree, when Sb/sub 2/O/sub 3/ was present. Cross sections of the bonds that show the Sb/sub 2/O/sub 3/-induced degradation and elemental analysis of the pulled ball-bonds suggest that the degradative reaction starts at the interface of the gold-rich intermetallic and the gold ball. Antimony trioxide appears to be associated with the Al portion of the Au-Al ball-bond intermetallics, and to be participating in the reactions or affecting the reactivity of Al in a high-moisture environment. These results contrast with several previous reports that Sb/sub 2/O/sub 3/ improves wire bond reliability in a dry environment.<<ETX>>","PeriodicalId":409540,"journal":{"name":"28th Annual Proceedings on Reliability Physics Symposium","volume":"47 1","pages":"0"},"PeriodicalIF":0.0000,"publicationDate":"1990-03-27","publicationTypes":"Journal Article","fieldsOfStudy":null,"isOpenAccess":false,"openAccessPdf":"","citationCount":"24","resultStr":"{\"title\":\"Effect of mold compound components on moisture-induced degradation of gold-aluminium bonds in epoxy encapsulated devices\",\"authors\":\"A. Gallo\",\"doi\":\"10.1109/RELPHY.1990.66095\",\"DOIUrl\":null,\"url\":null,\"abstract\":\"Degradation of the intermetallic region of the gold wire-aluminium bonding pad interface of several types of IC devices in plastic packages is accelerated by moisture at relatively low temperatures (121-135 degrees C), leading to near-complete loss of strength after 300-400 h of autoclave testing. Measurement of bonding strength as a function of steam-autoclave time in a designed experiment shows that one common component of semiconductor molding compounds (Sb/sub 2/O/sub 3/) is the overriding factor in causing ball-lift. In support of this conclusion, a variety of brominated flame retardants, including those that claimed to be more stable to Br release, were tested in similar formulations and all were found to give ball-bond degradation, to about the same degree, when Sb/sub 2/O/sub 3/ was present. Cross sections of the bonds that show the Sb/sub 2/O/sub 3/-induced degradation and elemental analysis of the pulled ball-bonds suggest that the degradative reaction starts at the interface of the gold-rich intermetallic and the gold ball. Antimony trioxide appears to be associated with the Al portion of the Au-Al ball-bond intermetallics, and to be participating in the reactions or affecting the reactivity of Al in a high-moisture environment. These results contrast with several previous reports that Sb/sub 2/O/sub 3/ improves wire bond reliability in a dry environment.<<ETX>>\",\"PeriodicalId\":409540,\"journal\":{\"name\":\"28th Annual Proceedings on Reliability Physics Symposium\",\"volume\":\"47 1\",\"pages\":\"0\"},\"PeriodicalIF\":0.0000,\"publicationDate\":\"1990-03-27\",\"publicationTypes\":\"Journal Article\",\"fieldsOfStudy\":null,\"isOpenAccess\":false,\"openAccessPdf\":\"\",\"citationCount\":\"24\",\"resultStr\":null,\"platform\":\"Semanticscholar\",\"paperid\":null,\"PeriodicalName\":\"28th Annual Proceedings on Reliability Physics Symposium\",\"FirstCategoryId\":\"1085\",\"ListUrlMain\":\"https://doi.org/10.1109/RELPHY.1990.66095\",\"RegionNum\":0,\"RegionCategory\":null,\"ArticlePicture\":[],\"TitleCN\":null,\"AbstractTextCN\":null,\"PMCID\":null,\"EPubDate\":\"\",\"PubModel\":\"\",\"JCR\":\"\",\"JCRName\":\"\",\"Score\":null,\"Total\":0}","platform":"Semanticscholar","paperid":null,"PeriodicalName":"28th Annual Proceedings on Reliability Physics Symposium","FirstCategoryId":"1085","ListUrlMain":"https://doi.org/10.1109/RELPHY.1990.66095","RegionNum":0,"RegionCategory":null,"ArticlePicture":[],"TitleCN":null,"AbstractTextCN":null,"PMCID":null,"EPubDate":"","PubModel":"","JCR":"","JCRName":"","Score":null,"Total":0}
Effect of mold compound components on moisture-induced degradation of gold-aluminium bonds in epoxy encapsulated devices
Degradation of the intermetallic region of the gold wire-aluminium bonding pad interface of several types of IC devices in plastic packages is accelerated by moisture at relatively low temperatures (121-135 degrees C), leading to near-complete loss of strength after 300-400 h of autoclave testing. Measurement of bonding strength as a function of steam-autoclave time in a designed experiment shows that one common component of semiconductor molding compounds (Sb/sub 2/O/sub 3/) is the overriding factor in causing ball-lift. In support of this conclusion, a variety of brominated flame retardants, including those that claimed to be more stable to Br release, were tested in similar formulations and all were found to give ball-bond degradation, to about the same degree, when Sb/sub 2/O/sub 3/ was present. Cross sections of the bonds that show the Sb/sub 2/O/sub 3/-induced degradation and elemental analysis of the pulled ball-bonds suggest that the degradative reaction starts at the interface of the gold-rich intermetallic and the gold ball. Antimony trioxide appears to be associated with the Al portion of the Au-Al ball-bond intermetallics, and to be participating in the reactions or affecting the reactivity of Al in a high-moisture environment. These results contrast with several previous reports that Sb/sub 2/O/sub 3/ improves wire bond reliability in a dry environment.<>