Shih-Hsien Chang, Kun-Jie Liao, K. Huang, Cheng Liang
{"title":"通过真空烧结工艺在 Ti-8Nb-4Co 合金中添加 Mo2C 粉末对微观结构和强化机制的影响","authors":"Shih-Hsien Chang, Kun-Jie Liao, K. Huang, Cheng Liang","doi":"10.24425/amm.2023.146190","DOIUrl":null,"url":null,"abstract":"This study utilizes Ti-8nb-4Co alloys added to different proportions of Mo 2 C powders (1, 3, and 5 mass%) by the vacuum sintering process of powder metallurgy and simultaneously vacuum sinters the alloys at 1240, 1270, 1300, and 1330°C for 1 h, respectively. The experimental results indicate that when 3 mass% Mo 2 C powders were added to the Ti-8nb-4Co alloys, the specimens possessed the optimal mechanical properties after sintering at 1300°C for 1 h. The relative density was 98.02%, and the hardness and TRS were enhanced to 69.6 hRa and 1816.7 MPa, respectively. in addition, the microstructure of vacuum sintered Ti-8nb-4Co-3Mo 2 C alloys has both α and β-phase structures, as well as TiC precipitates. EBSD results confirm that the Mo 2 C in situ produced TiC during the sintering process and was uniformly dispersed in the grain boundary. Moreover, the reduced molybdenum atom acted as a β-phase stabilizing element and solid-solution in the titanium matrix.","PeriodicalId":8304,"journal":{"name":"Archives of Metallurgy and Materials","volume":" 24","pages":""},"PeriodicalIF":0.7000,"publicationDate":"2023-12-19","publicationTypes":"Journal Article","fieldsOfStudy":null,"isOpenAccess":false,"openAccessPdf":"","citationCount":"0","resultStr":"{\"title\":\"Effects of the Microstructure and Strengthening Mechanisms of Mo2C Powders Being Added to Ti-8Nb-4Co Alloy Via the Vacuum Sintering Process\",\"authors\":\"Shih-Hsien Chang, Kun-Jie Liao, K. Huang, Cheng Liang\",\"doi\":\"10.24425/amm.2023.146190\",\"DOIUrl\":null,\"url\":null,\"abstract\":\"This study utilizes Ti-8nb-4Co alloys added to different proportions of Mo 2 C powders (1, 3, and 5 mass%) by the vacuum sintering process of powder metallurgy and simultaneously vacuum sinters the alloys at 1240, 1270, 1300, and 1330°C for 1 h, respectively. The experimental results indicate that when 3 mass% Mo 2 C powders were added to the Ti-8nb-4Co alloys, the specimens possessed the optimal mechanical properties after sintering at 1300°C for 1 h. The relative density was 98.02%, and the hardness and TRS were enhanced to 69.6 hRa and 1816.7 MPa, respectively. in addition, the microstructure of vacuum sintered Ti-8nb-4Co-3Mo 2 C alloys has both α and β-phase structures, as well as TiC precipitates. EBSD results confirm that the Mo 2 C in situ produced TiC during the sintering process and was uniformly dispersed in the grain boundary. Moreover, the reduced molybdenum atom acted as a β-phase stabilizing element and solid-solution in the titanium matrix.\",\"PeriodicalId\":8304,\"journal\":{\"name\":\"Archives of Metallurgy and Materials\",\"volume\":\" 24\",\"pages\":\"\"},\"PeriodicalIF\":0.7000,\"publicationDate\":\"2023-12-19\",\"publicationTypes\":\"Journal Article\",\"fieldsOfStudy\":null,\"isOpenAccess\":false,\"openAccessPdf\":\"\",\"citationCount\":\"0\",\"resultStr\":null,\"platform\":\"Semanticscholar\",\"paperid\":null,\"PeriodicalName\":\"Archives of Metallurgy and Materials\",\"FirstCategoryId\":\"88\",\"ListUrlMain\":\"https://doi.org/10.24425/amm.2023.146190\",\"RegionNum\":4,\"RegionCategory\":\"材料科学\",\"ArticlePicture\":[],\"TitleCN\":null,\"AbstractTextCN\":null,\"PMCID\":null,\"EPubDate\":\"\",\"PubModel\":\"\",\"JCR\":\"Q4\",\"JCRName\":\"METALLURGY & METALLURGICAL ENGINEERING\",\"Score\":null,\"Total\":0}","platform":"Semanticscholar","paperid":null,"PeriodicalName":"Archives of Metallurgy and Materials","FirstCategoryId":"88","ListUrlMain":"https://doi.org/10.24425/amm.2023.146190","RegionNum":4,"RegionCategory":"材料科学","ArticlePicture":[],"TitleCN":null,"AbstractTextCN":null,"PMCID":null,"EPubDate":"","PubModel":"","JCR":"Q4","JCRName":"METALLURGY & METALLURGICAL ENGINEERING","Score":null,"Total":0}
引用次数: 0
摘要
本研究利用粉末冶金的真空烧结工艺,在 Ti-8nb-4Co 合金中加入不同比例的 Mo 2 C 粉末(1、3 和 5 质量%),同时分别在 1240、1270、1300 和 1330°C 下真空烧结合金 1 小时。实验结果表明,当在 Ti-8nb-4Co 合金中添加 3 质量%的 Mo 2 C 粉末时,试样在 1300°C 下烧结 1 小时后具有最佳的机械性能,相对密度为 98.此外,真空烧结 Ti-8nb-4Co-3Mo 2 C 合金的微观结构具有 α 和 β 相结构以及 TiC 沉淀。EBSD 结果证实,Mo 2 C 在烧结过程中原位生成了 TiC,并均匀地分散在晶界中。此外,还原钼原子在钛基体中起到了β相稳定元素和固溶体的作用。
Effects of the Microstructure and Strengthening Mechanisms of Mo2C Powders Being Added to Ti-8Nb-4Co Alloy Via the Vacuum Sintering Process
This study utilizes Ti-8nb-4Co alloys added to different proportions of Mo 2 C powders (1, 3, and 5 mass%) by the vacuum sintering process of powder metallurgy and simultaneously vacuum sinters the alloys at 1240, 1270, 1300, and 1330°C for 1 h, respectively. The experimental results indicate that when 3 mass% Mo 2 C powders were added to the Ti-8nb-4Co alloys, the specimens possessed the optimal mechanical properties after sintering at 1300°C for 1 h. The relative density was 98.02%, and the hardness and TRS were enhanced to 69.6 hRa and 1816.7 MPa, respectively. in addition, the microstructure of vacuum sintered Ti-8nb-4Co-3Mo 2 C alloys has both α and β-phase structures, as well as TiC precipitates. EBSD results confirm that the Mo 2 C in situ produced TiC during the sintering process and was uniformly dispersed in the grain boundary. Moreover, the reduced molybdenum atom acted as a β-phase stabilizing element and solid-solution in the titanium matrix.
期刊介绍:
The Archives of Metallurgy and Materials is covered in the following Institute for Scientific Information products: SciSearch (the Science Citation Index - Expanded), Research Alert, Materials Science Citation Index, and Current Contents / Engineering, Computing and Technology.
Articles published in the Archives of Metallurgy and Materials are also indexed or abstracted by Cambridge Scientific Abstracts.