{"title":"论一次炼油设备安全阀弹簧过早失效的原因","authors":"M. A. Tupitsin, I. A. Trishkina, E. I. Storozheva","doi":"10.1134/s0020168524700213","DOIUrl":null,"url":null,"abstract":"<h3 data-test=\"abstract-sub-heading\">Abstract</h3><p>The reasons for the premature failure of a spring (made of 50KhFA steel) used in the safety valve of the column head part are analyzed. The failure of the spring occurred after 7 years of operation at a temperature below 90°C in a working environment of light oil products (sulfurous gasoline). Visual and measurement control, general chemical analysis of the composition of the steel, energy-dispersive analysis of the metal in local areas, measurements of hardness and microhardness, microstructural analysis of the metal, macro- and electron fractography, phase chemical and X-ray structural analyses, and recovering heat treatment are used for the studies. The characteristic external signs, typical microdamages, and mechanisms of sulfide (hydrogen) corrosion cracking of high-strength 50KhFA steel with the most dangerous accompanying process, hydrogenation, are revealed. The analysis of the chemical composition and hardness of the metal meets the requirements of the standards for this steel. The microstructure of the metal under study is tempered martensite with the presence of a decarburized layer of up to 0.158 mm in the surface layers. The results of the study show that the premature failure of the spring is attributed both to the technological heredity and operational factors (contact with the working environment beyond the design basis). Ulcerative damage of the metal surface with the penetration of corrosion products into the deep layers due to the violation of the integrity of the coating of the spring are noted, which indicates low resistance of 50KhFA steel to low-temperature hydrogen sulfide corrosion. The failure predominantly occurs near nonmetallic inclusions along the boundaries of the primary austenite grains, where the largest precipitates of chromium carbides are located, as well as along the interphase boundaries of oriented carbide plates.</p>","PeriodicalId":585,"journal":{"name":"Inorganic Materials","volume":"74 1","pages":""},"PeriodicalIF":0.9000,"publicationDate":"2024-07-30","publicationTypes":"Journal Article","fieldsOfStudy":null,"isOpenAccess":false,"openAccessPdf":"","citationCount":"0","resultStr":"{\"title\":\"On the Reasons for the Premature Failure of Safety Valve Springs in the Equipment of Primary Oil Refining\",\"authors\":\"M. A. Tupitsin, I. A. Trishkina, E. I. Storozheva\",\"doi\":\"10.1134/s0020168524700213\",\"DOIUrl\":null,\"url\":null,\"abstract\":\"<h3 data-test=\\\"abstract-sub-heading\\\">Abstract</h3><p>The reasons for the premature failure of a spring (made of 50KhFA steel) used in the safety valve of the column head part are analyzed. The failure of the spring occurred after 7 years of operation at a temperature below 90°C in a working environment of light oil products (sulfurous gasoline). Visual and measurement control, general chemical analysis of the composition of the steel, energy-dispersive analysis of the metal in local areas, measurements of hardness and microhardness, microstructural analysis of the metal, macro- and electron fractography, phase chemical and X-ray structural analyses, and recovering heat treatment are used for the studies. The characteristic external signs, typical microdamages, and mechanisms of sulfide (hydrogen) corrosion cracking of high-strength 50KhFA steel with the most dangerous accompanying process, hydrogenation, are revealed. The analysis of the chemical composition and hardness of the metal meets the requirements of the standards for this steel. The microstructure of the metal under study is tempered martensite with the presence of a decarburized layer of up to 0.158 mm in the surface layers. The results of the study show that the premature failure of the spring is attributed both to the technological heredity and operational factors (contact with the working environment beyond the design basis). Ulcerative damage of the metal surface with the penetration of corrosion products into the deep layers due to the violation of the integrity of the coating of the spring are noted, which indicates low resistance of 50KhFA steel to low-temperature hydrogen sulfide corrosion. The failure predominantly occurs near nonmetallic inclusions along the boundaries of the primary austenite grains, where the largest precipitates of chromium carbides are located, as well as along the interphase boundaries of oriented carbide plates.</p>\",\"PeriodicalId\":585,\"journal\":{\"name\":\"Inorganic Materials\",\"volume\":\"74 1\",\"pages\":\"\"},\"PeriodicalIF\":0.9000,\"publicationDate\":\"2024-07-30\",\"publicationTypes\":\"Journal Article\",\"fieldsOfStudy\":null,\"isOpenAccess\":false,\"openAccessPdf\":\"\",\"citationCount\":\"0\",\"resultStr\":null,\"platform\":\"Semanticscholar\",\"paperid\":null,\"PeriodicalName\":\"Inorganic Materials\",\"FirstCategoryId\":\"88\",\"ListUrlMain\":\"https://doi.org/10.1134/s0020168524700213\",\"RegionNum\":4,\"RegionCategory\":\"材料科学\",\"ArticlePicture\":[],\"TitleCN\":null,\"AbstractTextCN\":null,\"PMCID\":null,\"EPubDate\":\"\",\"PubModel\":\"\",\"JCR\":\"Q4\",\"JCRName\":\"MATERIALS SCIENCE, MULTIDISCIPLINARY\",\"Score\":null,\"Total\":0}","platform":"Semanticscholar","paperid":null,"PeriodicalName":"Inorganic Materials","FirstCategoryId":"88","ListUrlMain":"https://doi.org/10.1134/s0020168524700213","RegionNum":4,"RegionCategory":"材料科学","ArticlePicture":[],"TitleCN":null,"AbstractTextCN":null,"PMCID":null,"EPubDate":"","PubModel":"","JCR":"Q4","JCRName":"MATERIALS SCIENCE, MULTIDISCIPLINARY","Score":null,"Total":0}
引用次数: 0

摘要

摘要 分析了用于柱头部分安全阀的弹簧(由 50KhFA 钢制成)过早失效的原因。在轻质油品(含硫汽油)的工作环境中,弹簧在低于 90°C 的温度下工作 7 年后发生故障。研究中使用了目视和测量控制、钢成分的一般化学分析、金属局部区域的能量色散分析、硬度和显微硬度测量、金属的微观结构分析、宏观和电子分形、相化学和 X 射线结构分析以及恢复热处理。揭示了高强度 50KhFA 钢硫化物(氢)腐蚀开裂的外部特征、典型微损伤和机理,以及最危险的伴随过程--析氢。对金属化学成分和硬度的分析符合该钢种的标准要求。所研究金属的微观结构为回火马氏体,表层存在长达 0.158 毫米的脱碳层。研究结果表明,弹簧过早失效的原因既有技术遗传因素,也有操作因素(与工作环境的接触超出了设计基础)。由于弹簧涂层的完整性受到破坏,金属表面出现溃疡性损伤,腐蚀产物渗入深层,这表明 50KhFA 钢对低温硫化氢腐蚀的抵抗力较低。失效主要发生在沿初级奥氏体晶粒边界的非金属夹杂物附近(最大的铬碳化物析出物位于此处),以及沿取向碳化物板的相间边界。
本文章由计算机程序翻译,如有差异,请以英文原文为准。

摘要图片

查看原文
分享 分享
微信好友 朋友圈 QQ好友 复制链接
本刊更多论文
On the Reasons for the Premature Failure of Safety Valve Springs in the Equipment of Primary Oil Refining

Abstract

The reasons for the premature failure of a spring (made of 50KhFA steel) used in the safety valve of the column head part are analyzed. The failure of the spring occurred after 7 years of operation at a temperature below 90°C in a working environment of light oil products (sulfurous gasoline). Visual and measurement control, general chemical analysis of the composition of the steel, energy-dispersive analysis of the metal in local areas, measurements of hardness and microhardness, microstructural analysis of the metal, macro- and electron fractography, phase chemical and X-ray structural analyses, and recovering heat treatment are used for the studies. The characteristic external signs, typical microdamages, and mechanisms of sulfide (hydrogen) corrosion cracking of high-strength 50KhFA steel with the most dangerous accompanying process, hydrogenation, are revealed. The analysis of the chemical composition and hardness of the metal meets the requirements of the standards for this steel. The microstructure of the metal under study is tempered martensite with the presence of a decarburized layer of up to 0.158 mm in the surface layers. The results of the study show that the premature failure of the spring is attributed both to the technological heredity and operational factors (contact with the working environment beyond the design basis). Ulcerative damage of the metal surface with the penetration of corrosion products into the deep layers due to the violation of the integrity of the coating of the spring are noted, which indicates low resistance of 50KhFA steel to low-temperature hydrogen sulfide corrosion. The failure predominantly occurs near nonmetallic inclusions along the boundaries of the primary austenite grains, where the largest precipitates of chromium carbides are located, as well as along the interphase boundaries of oriented carbide plates.

求助全文
通过发布文献求助,成功后即可免费获取论文全文。 去求助
来源期刊
Inorganic Materials
Inorganic Materials 工程技术-材料科学:综合
CiteScore
1.40
自引率
25.00%
发文量
80
审稿时长
3-6 weeks
期刊介绍: Inorganic Materials is a journal that publishes reviews and original articles devoted to chemistry, physics, and applications of various inorganic materials including high-purity substances and materials. The journal discusses phase equilibria, including P–T–X diagrams, and the fundamentals of inorganic materials science, which determines preparatory conditions for compounds of various compositions with specified deviations from stoichiometry. Inorganic Materials is a multidisciplinary journal covering all classes of inorganic materials. The journal welcomes manuscripts from all countries in the English or Russian language.
期刊最新文献
Prediction of the Durability of a Plate with a Through Crack Taking into Account Biaxial Constraints of Deformations along the Front of a Normal Rupture Crack Refined Method for Estimating the Interlayer Shear Modulus by Correcting the Deflection of Polymer Composite Specimens Fields of Residual Stresses near Open Assemblage Holes of Aircraft Wing Panel On the Features of Inhomogeneous Residual Stress Identification Using the Digital Speckle Interferometry and the Hole-Drilling Method Actual Problems of Creating Digital Twins of Machine Engineering Products in Terms of Durability Assessment
×
引用
GB/T 7714-2015
复制
MLA
复制
APA
复制
导出至
BibTeX EndNote RefMan NoteFirst NoteExpress
×
×
提示
您的信息不完整,为了账户安全,请先补充。
现在去补充
×
提示
您因"违规操作"
具体请查看互助需知
我知道了
×
提示
现在去查看 取消
×
提示
确定
0
微信
客服QQ
Book学术公众号 扫码关注我们
反馈
×
意见反馈
请填写您的意见或建议
请填写您的手机或邮箱
已复制链接
已复制链接
快去分享给好友吧!
我知道了
×
扫码分享
扫码分享
Book学术官方微信
Book学术文献互助
Book学术文献互助群
群 号:481959085
Book学术
文献互助 智能选刊 最新文献 互助须知 联系我们:info@booksci.cn
Book学术提供免费学术资源搜索服务,方便国内外学者检索中英文文献。致力于提供最便捷和优质的服务体验。
Copyright © 2023 Book学术 All rights reserved.
ghs 京公网安备 11010802042870号 京ICP备2023020795号-1